Abstract:
This paper delves into the corrosion behavior and protection methods of magnesium alloys. The properties of magnesium, corrosion mechanisms, corrosion morphologies, and corrosion resistance comparison with other materials are discussed in detail. The electrochemical corrosion of magnesium alloys in neutral and alkaline environments is emphasized, along with various corrosion morphologies such as galvanic corrosion, pitting corrosion, stress corrosion, intergranular corrosion, and filamentary corrosion. The significant advancements in the development of high-purity magnesium alloys, such as AZ91D, are highlighted, which have significantly improved their corrosion resistance and made them suitable for various automotive applications without the need for additional protection.

Keywords:

magnesium alloys, corrosion, electrochemical corrosion, corrosion morphologies, high-purity alloys

  1. Properties of Magnesium

Magnesium, with the element symbol Mg and an atomic number of 12, has an electronic structure of 2-8-2. Its standard electrode potential is very negative (-2.36V), making it prone to losing electrons and undergoing oxidation reactions. Consequently, magnesium and its alloys exhibit poor corrosion resistance and are susceptible to severe corrosion in corrosive media. The naturally formed oxide film on magnesium alloys is porous and loose, with a density coefficient of around 0.8 (less than 1), primarily composed of MgO and Mg2+. This film provides poor protection to the substrate and is unsuitable for most corrosive environments.

  1. Corrosion Mechanisms of Magnesium Alloys

There are two primary types of corrosion mechanisms for magnesium alloys: general corrosion or environmental corrosion (also known as chemical corrosion) occurring in ordinary environments, and electrochemical corrosion occurring in galvanic cell environments.

When exposed to dry air, a thin film forms on the surface of magnesium alloys. This film remains stable without contact with water and corrosion does not occur. However, in practical operating environments, the film may come into contact with water or moisture, causing its color to darken (from light gray to dark gray). Further exposure to liquid water and air leads to the reaction with CO2 and H2O to form carbonates, thickening the film. In most cases, this film is stable and protective enough, eliminating the need for any additional treatment. For instance, the shells of automotive brakes do not require external protective measures.

Similarly, high-purity AZ91D alloys do not require protective measures. Even when in contact with splashed water from the road, these alloys remain protected as the film is stable and protective under neutral and alkaline conditions.

However, design flaws that allow water ingress or exposure to saline environment(such as seawater) can create a micro-battery environment, leading to severe electrochemical corrosion, even in neutral and alkaline environments. In such cases, a good surface treatment and protective measure are necessary.

Electrochemical corrosion is the primary mode of corrosion for magnesium alloys in neutral and alkaline environments. The principle of electrochemical corrosion in these environments is as follows (Figure 1):

Figure 1: Schematic Diagram of Electrochemical Corrosion

The chemical reaction mechanism is described by the following equations:

Mg-2e=Mg2+ (Anode reaction)

2H2O+2e=H2+OH- (Cathode reaction)

Mg2++2OH-=Mg(OH)2 (Corrosion product)

The overall reaction is Mg+2H2O= Mg(OH)2+ H2.

In this reaction, magnesium acts as the anode, losing electrons and undergoing corrosion, while hydrogen gas is released at the cathode. Typically, the cathode could be another metal component in contact with the magnesium alloy or alloying or impurity elements that form a galvanic cell with the magnesium alloy matrix, inducing electrode reactions and electrochemical corrosion.

  1. Corrosion Morphologies of Magnesium Alloys

The corrosion morphologies of magnesium alloys primarily include the following:

(i) Galvanic corrosion: This is the most common form of corrosion in magnesium alloys, where severe corrosion occurs in local regions adjacent to the cathode.

(ii) Pitting corrosion: In non-oxidizing media containing Cl-, magnesium alloys are prone to pitting corrosion under self-corrosion potentials. Similarly, pitting corrosion is also the predominant corrosion morphology in neutral or alkaline media.

(iii) Stress corrosion: Magnesium alloys have a tendency to corrode and crack in neutral solutions containing Cl-, even in distilled water. However, in alkaline media with a PH greater than 10.2, magnesium alloys exhibit good resistance to stress corrosion. Similarly, they also demonstrate good resistance in fluoride solutions.

(iv) Intergranular corrosion: Magnesium alloys are generally insensitive to intergranular corrosion, and corrosion does not develop along grain boundaries.

(V) Filiform Corrosion: Filiform corrosion occurs under protective organic coatings or anodic oxide films due to the movement of corrosion cells on the surface of magnesium alloy substrates.

  1. Comparison of Corrosion Resistance between Magnesium Alloys and Other Materials

Significant progress was made in the development of magnesium alloy materials in the 1980s. It was discovered that impurity elements such as Fe, Ni, Cu, and the ratio of Fe to Mn have a significant impact on the corrosion resistance of magnesium alloys. Consequently, a new generation of high-purity die-cast magnesium alloys, such as AZ91D, was developed. The corrosion resistance of high-purity magnesium alloys has been improved by a factor of 100, surpassing other competing materials. Without any protective coatings, they can meet the requirements of most automotive applications, even under winter road conditions. This technological breakthrough is crucial for the later development of die-cast magnesium alloys and is a significant reason for their widespread application. In terms of salt spray corrosion resistance, most die-cast magnesium alloy grades have surpassed aluminum alloy A380 (as shown in Figure 2).

Figure 2: Comparison of Salt Spray Corrosion Tendencies between Magnesium Alloy and Aluminum Alloy A380

 
 
  1. Corrosion Protection Technologies for Magnesium Alloys

Based on the corrosion mechanisms of magnesium alloys, current research on corrosion protection technologies for magnesium alloys mainly focuses on the following aspects:

5.1 Part Design (as shown in Figure 3)

A good protection measure starts with a good design. This is a systematic engineering approach. From the perspective of corrosion protection, a good magnesium alloy part design should consider the following factors:

(1) Prevent water or other liquids from accumulating and forming a galvanic cell environment.

(2) Design rounded corners as sharp corners can reduce protective effects.

5.2 Material Selection (as shown in Figure 3)

In product design, the selection of raw materials for adjacent components is also crucial. It is necessary to ensure that both the structural functionality is unaffected and the potential difference between the two materials is small to prevent severe corrosion.

Another important aspect is the materials used for connecting parts and connecting media, as well as the corrosion protection treatment processes.

Figure 3: Corrosion Protection Methods for Magnesium Alloys

Below is a list of the electrochemical activity sequence of some commonly used materials (at room temperature, in seawater). Materials closer to magnesium have better compatibility with it:

Magnesium

Magnesium Alloys

Aluminum Alloys 5000, 30000, 1100, 6000

Cadmium

Aluminum Alloys 2000

Steel

13% Chromium-plated Stainless Steel (Active)

18-8 Unplated Steel (Active)

Aluminum

Zinc

Naval Brass

Nickel (Active)

Aluminum-Copper Alloy

Red Copper, Copper

Nickel (Inert)

Nickel-Copper Alloy

Titanium

18-8 Stainless Steel (Inert)

Gold

5.3 Metallurgical Control

Metallurgical factors include alloy components, impurity elements, phase composition, and microstructure.

Different elements have different effects on the corrosion performance of magnesium alloys. Based on the commonly used alloy components of magnesium alloy materials, they are generally divided into three categories, as shown in Table 1. By analyzing the effects of alloy elements on the corrosion rate of magnesium alloys, the content of the third category of elements is usually reduced to below the critical value, and the corrosion resistance is increased by improving purity.

Elements with minor effects on corrosion rate: Al, Mn, Na, Si, Zr, etc.

Elements with slightly greater effects on corrosion rate: Zn, Cd, Ca, Ag, etc.

Elements with extremely increased effects on corrosion rate: Ni, Fe, Cu, Co, etc.