News
Failure Solutions for Surface Enhancement Treatment of Die Casting Molds
Abstract:
Die casting molds are subjected to extreme operating conditions during production, including temperatures ranging from 680 to 720°C and pressures up to 200 MPa. Surface erosion and fracture are the primary causes of mold failure, significantly impacting mold lifespan. To address these issues, surface treatment methods have been employed to enhance the surface properties of mold cores. This paper presents an overview of common failure modes in die casting molds and corresponding solutions developed by ASSAB Shanghai Company through extensive research, experimentation, and production practice. Six innovative surface treatment processes (ABP, ASO, ASN, ABP+ASN, ABP+ASO, ASN+ASO) introduced since April 2006 are highlighted, focusing on their mechanisms, causes, and effective mitigation strategies.
Keywords: Die casting mold, surface treatment, erosion, corrosion, thermal fatigue cracking, adhesion, ABP, ASO, ASN
Failure Modes and Solutions for Die Casting Molds
Die casting molds experience various failure modes, including erosion, corrosion, thermal fatigue cracking, adhesion, and cracking. Effective solutions have been devised to mitigate these issues and enhance mold durability.

I. Erosion Mechanism and Solutions
Mechanism: Erosion results from high-speed friction between the mold and hot liquid alloy, causing surface wear.
Causes:
Wear between the liquid alloy and mold surface.
Insufficient wear resistance of the mold surface.
Excessive pressure, flow rate, and temperature.
Solutions:
Reduce non-metallic content (e.g., Si impurities) in alloy materials.
Employ wear-resistant die casting mold materials and apply surface treatments (e.g., ASN) to enhance surface wear resistance without compromising toughness.
Decrease pressure, flow rate, and alloy temperature.
II. Corrosion Mechanism and Solutions
Mechanism: Corrosion occurs due to chemical reactions between the molten alloy and mold surface.
Causes:
Formation of intermetallic compounds through chemical reactions between the alloy and mold.
High-temperature alloy metal vapor corroding the mold surface.
Solutions:
Prevent direct contact between the mold and high-temperature alloy metal using surface treatments like ASO to isolate Fe from reacting with Al, Zn, etc.
Design efficient cooling water channels to reduce mold surface temperature.

III. Thermal Fatigue Cracking Mechanism and Solutions
Mechanism: Thermal fatigue cracking arises from alternating thermal stresses exceeding the mold's fatigue strength, leading to surface microcracks.
Causes:
Choice of mold material.
Elevated mold surface temperatures.
Stress induced by repeated heating and cooling cycles.
Solutions:
Select mold materials with high strength, hardness, and toughness at high temperatures (e.g., DIEVAR, 8407).
Implement efficient cooling systems to reduce mold surface temperatures.
Enhance surface compressive stress, refine surface grain structure, and increase surface hardness through treatments like ABP.
IV. Adhesion Mechanism and Solutions
Mechanism: Adhesion occurs when the die-cast product bonds to the mold, damaging both surfaces.
Causes:
Inconsistent application of release agent on the mold surface.
Surface damage to the mold.
Low surface hardness of the mold.
Solutions:
Maintain a certain level of roughness on the mold surface to facilitate uniform release agent adhesion (ABP treatment).
Increase surface hardness and strength through treatments like ASN.
ASSAB Surface Enhancement Treatment Definitions
|
Process |
Definition |
Characteristics |
|
ABP |
ASSAB blasting (shot) peening |
1. Induces compressive stress on the mold surface.<br>2. Refines surface structure.<br>3. Enhances surface strength.<br>4. Improves surface hardness. |
|
ASO |
ASSAB steam oxidation |
1. Forms an Fe3O4 oxide film isolating the molten alloy from the mold.<br>2. The scaly oxide film facilitates retention of release agents. |
|
ASN |
ASSAB special nitriding |
1. Provides a high-hardness, wear-resistant nitride layer without compromising mold toughness.<br>2. Avoids the formation of a brittle white layer, reducing cracking risks. |
This comprehensive approach to addressing die casting mold failures through advanced surface treatments underscores the critical role of material science and surface engineering in enhancing mold performance and longevity.