News

Calculation Methods of Pressure and Speed in Die Casting Process

Pressure is a fundamental characteristic of the die casting process, as the filling and compaction of molten metal are accomplished under its action. Pressure is divided into dynamic injection pressure and pressure boosting injection pressure. The dynamic injection pressure serves to overcome various resistances and ensure that the molten metal reaches a certain velocity during filling. The pressure boosting injection pressure, on the other hand, is used to compact the casting after filling, increasing its density and enhancing the clarity of its contours. The injection pressure is applied to the molten metal through the injection plunger, and the magnitude of the applied pressure is expressed as specific pressure. The dynamic injection specific pressure for cold chamber die casting machines typically ranges from 30-90 MPa, while the pressure boosting injection specific pressure ranges from 50-300 MPa. Hot chamber die casting machines can provide injection specific pressures up to 20-50 MPa. It should be noted that the maximum injection specific pressure can only be achieved using the smallest injection plunger provided by the die casting machine. When selecting the injection specific pressure, consideration should be given to the injection force capable of being delivered by the die casting machine and the plunger used, as exceeding the selectable range will not be achievable.

  1. Injection Specific Pressure

The relationship curve between boosting time and pressure during die casting is as follows:

 

Note:

t1 - Time during which the molten metal is not under pressure in the injection chamber; P1 represents the first stage (slow speed)

t2 - Time taken for the molten metal to fill the mold cavity through the ingate under the action of the injection plunger in the injection chamber; P2 represents the second stage (fast speed)

t3 - Moment just after the filling is completed; P3 represents the third stage (pressure boosting)

t4 - Final static pressure; P4 is used for supplementary compaction of the casting

 

The selection of specific pressure is influenced by various factors, and generally, the following principles should be followed:

  1. Structural characteristics of the casting. ① For thin-walled castings, a higher injection specific pressure can be selected; for castings with varying thicknesses, a higher pressure boosting specific pressure may be appropriate. ② Complex shapes may require a higher injection specific pressure. ③ Good processability may allow for a lower injection specific pressure.
  2. Properties of the die casting alloy. ① A wider crystallization temperature range may necessitate a higher pressure boosting specific pressure. ② Poor fluidity may require a higher injection specific pressure. ③ A higher density may require both a higher injection and pressure boosting specific pressure.
  3. Gating system. ① Longer flow paths, multiple turns, thin gates, and high resistance may necessitate a higher injection specific pressure. ② A flat runner with fast heat dissipation may require a higher injection specific pressure.
  4. Temperature of the alloy and die casting mold. ① Lower alloy pouring temperatures and die casting mold temperatures may require a higher injection specific pressure. ② When there is a significant temperature difference between the molten alloy and the die casting mold, a higher injection specific pressure may be needed.
  5. Quality of the die casting. ① High internal quality requirements for the casting may necessitate a higher pressure boosting specific pressure. ② High surface quality requirements for the casting may require a higher injection specific pressure.
  1. Mold Filling Force

During the die casting process, under the action of specific pressure, the molten metal fills the cavity, exerting a certain pressure on the cavity wall and parting surface. This pressure is known as the mold filling force. At the final stage of die casting, when the boost pressure is transmitted to the die casting mold through the molten metal, the mold filling force reaches its maximum. It is an important parameter for the initial selection of die casting machine models and the verification of strength and stiffness of the support plate for die casting parts. The mold filling force can be initially estimated based on the area of the parting surface using the following formula:

Fz = pbA

Where:

Fz ---- Mold filling force on the parting surface (N). When there is a movable insert clamping device, the component force in the locking direction caused by the lateral mold filling force should be taken into account.

Pb ---- Injection specific pressure (MPa). Boost pressure should be used for die casting machines equipped with boost mechanism.

A ---- Total projected area of the die casting part, gate, and venting system on the parting surface.

Table 1: Common Specific Pressures for Various Die Casting Alloys

Alloy

Casting Wall Thickness ≤ 3 (mm)

Casting Wall Thickness > 3 (mm)

Simple Structure

Complex Structure

Simple Structure

Complex Structure

Zinc Alloy

20-30

30-40

40-50

50-60

 

 

Aluminum-Silicon, Aluminum-Copper Alloy

25-35

35-45

45-60

60-70

 

 

Aluminum, Magnesium Alloy

30-40

40-50

50-65

65-75

 

 

Magnesium Alloy

30-40

40-50

50-65

65-80

 

 

Copper Alloy

40-50

50-60

60-70

70-80

 

 

 

Note: The specific pressure ranges provided in the table are typical values and may vary depending on the actual die casting conditions and the desired properties of the casting parts. It is recommended to consult with die casting manufacturers or refer to industry standards for specific applications.

  1. Velocity

During the die casting process, velocity is directly influenced by pressure and jointly plays a significant role in internal quality and surface contour clarity. Velocity can be classified into two forms: injection velocity and ingate velocity.

  1. Injection Velocity

Injection velocity, also known as plunger velocity, refers to the movement speed of the metal liquid pushed by the injection plunger within the injection chamber. The injection velocity varies during the injection process and can be divided into two stages: low-speed and high-speed. These stages can be adjusted seamlessly through the speed control valve of the die casting machine.

The first and second stages of injection involve low-speed injection, which prevents the metal liquid from spilling out of the feed port. This also allows sufficient time for the air within the injection chamber to escape and allows the metal liquid to accumulate at the forefront of the ingate. The low-speed injection velocity is determined based on the amount of metal liquid poured into the injection chamber. The third stage is high-speed injection, which allows the metal liquid to rapidly fill the mold cavity after passing through the ingate. This creates a pressure peak that compacts the casting, eliminating or reducing shrinkage porosity and shrinkage.

Table 2: Selection of Low-Speed Injection Velocity

Chamber Fill Rate (%)

Injection Velocity (cm/s)

≤30

30–40

30–60

20–30

>30

10–20

  1. Ingate Velocity

Ingate velocity refers to the linear velocity of the metal liquid entering the mold cavity through the ingate. A higher ingate velocity enables the metal liquid to rapidly fill the mold cavity before solidification, even with lower specific pressure, resulting in castings with clear contours and smooth surfaces. It also enhances the dynamic pressure of the metal liquid.

However, an excessively high ingate velocity can lead to a series of issues, including the entrapment of gas bubbles, the metal liquid entering the mold cavity in a mist-like form, and adhesion to the mold cavity wall, which can prevent subsequent metal liquid from fusing and result in surface defects and oxide inclusions. This can also accelerate the wear of the die casting mold.

When selecting the ingate velocity, the following factors should be considered:

  1. For complex shapes or thin-walled castings, a higher ingate velocity is preferred.
  2. When the alloy pouring temperature is low, a higher ingate velocity can be used.
  3. If the alloy and mold materials have good thermal conductivity, a higher ingate velocity is recommended.
  4. A thicker ingate thickness necessitates a higher ingate velocity.

Too low an ingate velocity can result in unclear casting contours, while too high a velocity can cause defects such as porosity in the casting. The relationship between ingate velocity, the average wall thickness of the casting, and the filling time is summarized in Table 3.

 

Table 3:  Recommended  Ingate Velocity of Die Castings

Average Wall Thickness of Casting (mm)

Filling Time (ms)

Ingate Velocity (m/s)

1

10–14

46–55

1.5

14–20

44–53

2

18–26

42–50

2.5

22–32

40–48

3

28–40

38–46

3.5

34–50

36–44

4

40–60

34–42

5

48–72

32–40

 

  1. Relationship between the Velocity of the Ingate and the Injection Speed and Pressure
    In a cold chamber die casting machine, the pressure chamber, runner, and die casting mold constitute a closed system. According to the principle of continuity, there is a fixed relationship between the velocity of the ingate and the injection speed. Namely,
    AnVn = d²Vy/4

Where:
d ---- Diameter of the pressure chamber (cm);
Vy ---- Injection speed (cm/s);
An ---- Cross-sectional area of the ingate (cm²);S
Vn ---- Velocity of the ingate (cm/s).